Intercontinental Casting — Integrated Supply Chain Platform for Non-standard Casting Parts

Process and Quality Control of Melting Gray Iron in Medium-Frequency Induction Furnace

Publication Date : 2022-09-20 09:53:42

Process and Quality Control of Melting Gray Iron in a Medium-Frequency Induction Furnace

Duan Pingchang, Huang Tao

(China National Building Material Group, Kaisheng Heavy Industry Co., Ltd., Huainan 232008, Anhui)

Source: Foundry Technology

 

Abstract:In view of the characteristics of melting gray iron in a medium-frequency induction furnace and the characteristics of electric furnace molten iron, the effects of raw material selection, charge ratio, chemical composition, carburization rate, melting temperature, and inoculation treatment on the strength and other properties of gray iron were analyzed. The process, quality control, and improvements of molten iron for melting gray iron in a medium-frequency induction furnace were described, and the importance of high-purity molten iron for ensuring the high quality and high performance of gray iron castings was proposed. The results show that through process improvements, it is possible to improve gray iron castings quality and performance, reduce or eliminate casting defects, and lower the reject rate.

Keywords:Gray iron; medium-frequency induction furnace melting; quality control

CLC number:TG243   Document code:A   Article number:1000-8365(2020)05-0450-06

DOI:10.16410/j.issn1000-8365.2020.05.010

 

Melting technology and Quality Control of Gray Cast Iron in Intermediate Frequency Induction Furnace

DUAN Pingchang, HUANG Tao

(CNBM Triumph Heavy Industries Co., Ltd., Huainan 232008, China)

 

Abstract: According to the characteristics of medium frequency induction furnace melting gray cast iron and the characteristics of electric molten iron, the effects of raw materials selection, charge ratio, chemical composition, carbon rate, melting temperature and inoculation treatment on the strength and performance of gray cast iron were analyzed. The process, quality control and improvement of melting molten iron of gray cast iron in intermediate frequency induction furnace were described. The results show that the quality and performance of gray cast iron castings can be improved, the casting defects can be reduced or eliminated, and the reject rate can be reduced.

Key words: gray cast iron; intermediate frequency furnace melting; quality control

 

In the current cast iron production of foundry enterprises, cupola melting has mostly been shut down because it is difficult for environmental protection to meet standards, and foundry enterprises now mostly use medium-frequency induction furnaces to melt cast iron. Compared with cupolas, the medium-frequency induction furnace melting process is relatively simple; the chemical composition and temperature of molten iron are easy to control, with no carbon pick-up and no sulfur pick-up, which is conducive to obtaining low-sulfur molten iron; environmental pollution is small, and the working environment and labor intensity of front-furnace smelting are also greatly improved; by using the nighttime electricity price trough for melting, production costs can be controlled to be roughly equivalent to those of cupola melting; for molten iron of the same chemical composition and castings poured in the same mold, gray iron melted in a medium-frequency induction furnace has higher strength and hardness than that melted in a cupola; molten iron from a medium-frequency induction furnace has a higher superheat temperature and poorer fluidity than cupola molten iron, and has the following adverse characteristics: the number of crystal nuclei in the molten iron is small; the degree of undercooling, chilling tendency, and shrinkage tendency are large; thick-walled parts of castings are prone to shrinkage cavities and shrinkage porosity, and thin-walled parts are prone to casting defects such as chill and hard edges. In hypoeutectic gray cast iron,The amount of Type A graphite is very liable to decrease, while the amount of Type D and E graphite and the associated ferrite increases, and the amount of pearlite is small. All of these, together with some other improper factors existing in daily production, are manifested in production as fluctuations in casting quality and affect the normal production of cast iron. In response to the new problems arising from melting gray iron in a medium-frequency induction furnace, the author overcame many difficulties such as the scarcity of technical data on electric furnace melting of gray iron and the great difficulty of practice and exploration, gradually explored and summarized some production technical experience and insights, hoping to provide help to small and medium-sized foundry enterprises that are in the throes of difficult operation and transformation and upgrading.

 

1 Selection of Raw Materials and Charge Ratio

The quality of the charge materials used directly affects the quality of the molten iron. Melting gray iron in a medium-frequency induction furnace has relatively high requirements for the cleanliness and dryness of charge materials. If the charge materials are not clean, contain harmful elements, or melting control is improper, it will cause oxidation of the molten iron and low purity, seriously deteriorate the metallurgical quality of the molten iron, affect the matrix structure and graphite morphology of the cast iron, and cause problems such as poor inoculation, large chilling and shrinkage porosity tendencies, and many gas holes. Therefore, the management of raw and auxiliary materials should be strengthened, and charge materials that are severely rusted or stained with oil must be prohibited. At the same time, in order to improve the purity of the molten iron and stabilize the chemical composition of the molten iron, carbon steel scrap should be selected as charge material and should account for more than half of the charge ratio; for foundry returns, gates and risers of castings of the same material should be selected, and the adhering molding sand and coating should be cleaned off before use. The usage amount should beabout 40%; scrap iron turnings should also be machining turnings of castings of the same material; for pig iron, because the impurities, trace elements, and structural defects therein are hereditary, pig iron with a stable source, clean and less rusty, low content of harmful elements, and preferably grade Z18 or above foundry pig iron should be selected. Castings produced from such pig iron have good and stable internal quality. Do not easily change the source of pig iron; otherwise, quality problems that may be caused by using charge materials with unqualified factors will be impossible to guard against. In addition, pig iron should preferably be added in the early stage of melting, and its ratio can be about 15%, which is beneficial to improving the graphite morphology of cast iron; for the carburizer, commercial graphite carburizer or carburizer that has undergone high-temperature graphitization treatment should be selected, and it should be added as early as possible during melting so that the carburizer is in direct contact with the molten iron and has sufficient time to melt and be absorbed; ferroalloys and inoculants should have qualified chemical composition, suitable particle size, and be appropriately preheated before use. During batching, the contents of elements such as C, Si, and Mn should be calculated in advance according to the charge ratio and material composition, and the insufficient parts should be adjusted with carburizer and ferroalloys. During composition fine-tuning in the later stage of melting, if the C content is low, pig iron can be added for carburization; if the C content is high, low-carbon steel scrap can be added to reduce carbon.

 

2 Effects of Chemical Composition

Carbon and silicon are strongly graphitizing elements,If C and Si are too high, it will lead to graphite coarsening, increased ferrite content, and reduced pearlite content, and the strength and hardness of cast iron will decrease. The strength of the cast iron matrix increases with increasing pearlite content[1], therefore, in high-strength gray cast iron,the C and Si contents should be appropriately reduced within a certain range. While ensuring the achievement of a gray fracture, this is conducive to refining graphite, promoting the formation of pearlite, and improving mechanical properties. Carbon equivalent CE and Si/C ratio significantly affect the structure and properties of gray cast iron. Selecting appropriate CE and Si/C ratio is beneficial for improving the structure and properties of cast iron. CE is the most important factor affecting the internal quality of gray iron castings. Increasing CE can greatly improve the casting performance of cast iron, reduce chill, shrinkage cavities, shrinkage porosity, and leakage defects, and lower the reject rate; this is particularly important for thin-walled cast iron parts. However, if CE is too high, the amount of precipitated graphite increases, the tendency to ferritization is obvious, and the tensile strength and hardness of castings are reduced. At thick-walled parts of castings, due to slow cooling rate, coarse grains and loose structure defects are likely to occur; if CE is too low, local hard zones are likely to form at thin-walled parts of castings, resulting in poor machining performance. Due to low CE, eutectic ledeburite and Type D and E undercooled graphite are likely to appear in the gray cast iron structure, resulting in reduced casting performance, increased section sensitivity of castings, increased internal stress, and increased hardness. Appropriately increasing the Si/C ratio can increase the strength of cast iron and improve the machinability of cast iron. Under the same conditions, different Si/C ratios can cause relatively large differences in the mechanical properties and structure of cast iron. When CE is constant, as the Si/C value increases from 0.6 to 0.8, the strength and hardness of gray iron reach a peak; when the Si/C value is constant, the strength and hardness of gray iron decrease with increasing CE. While strictly controlling CE at the production site, an appropriate Si/C ratio should be selected and controlled. The CE of gray iron melted in a medium-frequency induction furnace should be about 0.3% higher than that of the same grade gray iron melted in a cupola, the C content should be about 0.1% higher than that melted in a cupola, and the Si/C ratio should be controlled at 0.6–0.7, so that the cast iron maintains suitable hardness and relatively high tensile strength.

Manganese and sulfur are elements that stabilize pearlite and hinder graphitization. Manganese can promote and refine pearlite; an increase in manganese content can increase the strength and hardness of cast iron as well as the pearlite content in the structure; manganese can promote the formation and stabilization of carbides and can inhibitthe formation of FeS. Manganese also forms high-melting-point compounds with sulfur as heterogeneous nuclei and refines grains, so the amount of manganese used in high-grade gray cast iron is increased. However, if the manganese content is too high, it affects nucleation during molten iron crystallization, reduces the number of eutectic cells, causes coarse graphite, and produces undercooled graphite, which instead reduces the strength of cast iron. Sulfur is a restricted element in gray cast iron. An appropriate amount of sulfur plays a positive and beneficial role in the nucleation and growth of graphite and can improve the inoculation effect and machining performance of gray cast iron. For melting gray cast iron in a medium-frequency induction furnace, in order to ensure the inoculation effect, w(S) ≥ 0.06% is generally required, but preferably ≤ 0.08%. Phosphorus is generally a harmful element in gray cast iron and easily forms low-melting-point phosphide eutectic at grain boundaries, causing cold cracking of cast iron. Therefore, in gray cast iron, phosphorus is generally as low as possible. For cast iron parts with tightness requirements, the phosphorus content should be lower than 0.06%.

In actual production, the chemical composition design should be optimized according to factors such as the grade, wall thickness, size, and structural complexity of different Gray Iron castings, and the fluctuation range of each element should be strictly controlled. This is very critical to ensuring the quality and performance of Gray Iron castings.

 

3 Process, Quality Control and Improvement of Melting Gray Iron in Medium-Frequency Induction Furnaces

3.1 Control of Recarburization Rate and Use of Recarburizer

When melting gray iron in a medium-frequency induction furnace, many people believe that as long as the chemical composition and temperature of the molten iron are controlled before the furnace, high-quality molten iron can be melted, but this is not the case. The top priority in melting gray iron in a medium-frequency induction furnace is to control the core role of the recarburizer, and the core technology is recarburization of the molten iron. The higher the recarburization rate, the better the metallurgical properties of the molten iron. The recarburization rate mentioned here refers to carbon added to the molten iron in the form of a recarburizer, not carbon brought in by the charge materials. Production practice shows that in the charge ratio, a high proportion of pig iron leads to a large chill tendency; an increased proportion of recarburizer reduces the chill tendency. This requires using more cheap scrap steel and foundry returns in the charge, and using less or no new pig iron. In the molten iron using the scrap steel recarburization process, there are a large number of fine, dispersed heterogeneous nuclei, which can reduce the undercooling of the molten iron, promoting theformation of graphite structures dominated by Type A graphite[3]. At the same time, the reduction in pig iron usage also reduces the adverse hereditary effect of coarse graphite in pig iron, and the performance of gray iron also improves with increasing scrap steel usage. In actual production, it has been found that when the scrap steel usage is about30%, with the same scrap steel, foundry returns, and new pig iron as charge materials, when the chemical composition is basically the same, the gray iron melted in a medium-frequency induction furnace has lower performance than that melted in a cupola, and the strengthening inoculation effect is not obvious. This is due to the low scrap steel usage and low recarburization rate. This shows the importance of recarburization for ensuring the molten iron quality of gray iron and improving the structure and performance of gray iron.

The performance of gray iron is determined by the matrix structure and the morphology, size, quantity, and distribution of graphite. Changing graphite morphology is an important way to change the performance of cast iron. Comparatively speaking, the matrix structure is easier to control, and it mainly depends on the chemical composition and cooling rate of the molten iron. However, graphite morphology is not easy to control, and it requires a good degree of graphitization of the cast iron. Strangely, only newly added carbon participates in graphitization, while the original carbon in the charge materials does not participate in graphitization. If no recarburizer is used, although the melted molten iron has qualified chemical composition, suitable temperature, and reasonable inoculation, its performance is unsatisfactory: it appears to have a relatively high temperature, but its fluidity is not very good, the tendency to shrinkage cavities and shrinkage porosity is large, it easily absorbs gas, easily produces chill, has high section sensitivity, and contains many inclusions in the molten iron. All these are caused by the low recarburization rate and low degree of graphitization of the molten iron.

The forms of carbon in the original molten iron are mainly fine graphite and carbon atoms. From the perspective of refining graphite, too many carbon atoms are undesirable in the original molten iron, as they will inevitably reduce the number of graphite nuclei, and carbon atoms are more likely to form cementite during cooling, whereas fine graphite can directly serve as heterogeneous nucleation cores. Refining graphite and increasing nuclei are key to achieving high performance of cast iron. Increasing the amount of recarburizer can increase the number of nucleation cores, thereby laying a solid foundation for refining graphite. Therefore, in actual production, emphasis should be placed on the use of recarburizer and the recarburization effect:① The absorption rate of the recarburizer is directly related to its C content; the higher the C content, the higher the absorption rate; ② The particle size of the recarburizer is the main factor affecting its dissolution into the molten iron. Practice has proved that the particle size of the recarburizer should preferably be 1–4 mm; both fine powder and coarse particles have poor recarburization effects; ③ Silicon has a great influence on the recarburization effect. High-silicon molten iron has poor recarburization ability and slow recarburization speed, so ferrosilicon should be added after recarburization is in place, and the principle of recarburization first and silicon addition later should be followed; ④ Sulfur can hinder the absorption of carbon. The recarburization speed of high-sulfur molten iron is much slower than that of low-sulfur molten iron; ⑤ Graphite recarburizer can improve the nucleation ability of molten iron, and its absorption rate is also more than 10% higher than that of non-graphite recarburizer, so low-nitrogen graphite recarburizer should be selected; ⑥ The recommended method of using recarburizer is the furnace-charging method, that is, first add a certain amount of small pieces of foundry returns and scrap steel to the furnace bottom, then add all the recarburizer required according to the charge amount, press a layer of small pieces of scrap steel and pig iron on top, and then continue to add charge materials while melting. This method is simple and easy to implement, has high production efficiency, and the absorption rate can reach 90%. If the amount of recarburizer added is very large, it can be added in two batches: first add 60%–70% on the scrap steel bedding layer at the furnace bottom, and add the rest while continuing to add scrap steel. Recarburizer can also be added when the molten iron temperature is 1400–1430°C, with the goal of increasing the C content of the molten iron to the upper limit required by the grade; ⑦ The recarburizer should not be added too late. Adding recarburizer in the later stage of melting has two disadvantages: first, the recarburizer is easily burned off, and the carbon absorption rate is very low. Second, the recarburizer added later requires additional melting and absorption time, delaying chemical composition adjustment and heating time, reducing production efficiency, increasing power consumption, and possibly causing harm due to excessive heating; ⑧ Stirring of the molten iron can promote recarburization, especially for graphite clusters attached to the furnace wall. If excessive heating and a certain period of molten iron holding are not used, they are not easily dissolved into the molten iron. The relatively strong electromagnetic stirring of the medium-frequency induction furnace is beneficial to recarburization.

3.2 Temperature Control

The temperature during the melting period of gray iron should not be too high, and is generally controlled atbelow 1400°C. If the melting temperature is too high, alloy burning loss or reduction will affect composition adjustment in the later stage of melting. After the charge is completely melted and the furnace temperature reaches 1460°C, take a sample for rapid testing, then skim off all slag, and then add the remaining charge materials such as ferroalloys. The effect of slag removal temperature on molten iron quality is closely related to stable chemical composition and inoculation effect, and directly affects the control of tapping temperature. If the slag removal temperature is too high, it will intensify the burning loss of graphite nuclei in the molten iron and the reduction of silicon to a higher level (in an acidic lining), and produce a carbon-removal effect, affecting crystallization according to the stable system; if the slag removal temperature is too low, the molten iron is exposed for a long time, C and Si burn losses are severe, the composition needs to be adjusted again, the smelting time is prolonged, and the molten iron is overheated, increasing undercooling, making it easy for the composition to run out of control and destroying normal crystallization.

Tapping temperature control must ensure the optimal temperature for inoculation treatment and pouring; generally, according to actual conditions, the tapping temperature should be controlled at1460–1500°C, and the superheating temperature can be controlled at 1510–1530°C, followed by holding for 5–8 min. Within 1500–1550°C, increasing the superheating temperature of the molten iron and extending the high-temperature holding time will refine graphite and the matrix structure, improve the strength of cast iron, facilitate inoculation treatment, and eliminate gas porosity, inclusion defects, and the adverse effects of charge material heredity on the structure and performance of cast iron. If the holding temperature is too low and the time is too short, the recarburizer cannot completely dissolve into the molten iron, and it is also unfavorable for impurities in the molten iron to float up and be removed by slag skimming. However, if the superheating temperature is too high or the high-temperature holding time is too long, it will instead deteriorate graphite morphology, coarsen the matrix, increase undercooling, increase chill tendency, cause the existing heterogeneous nuclei in the molten iron to disappear, cause severe oxidation, reduce the performance of cast iron, and affect the control of tapping temperature. If the tapping temperature is too high, even though the C and Si contents are moderate, the chill depth of the poured triangular test block will be too large, or mottling will appear in the central part. If this occurs, the medium-frequency power should be reduced, and pig iron should be added to the furnace to lower the temperature and increase carbon.

Pouring temperature should also not be too high; otherwise, it will cause severe sand burning defects on castings, and some may even be difficult to clean, causing the castings to be scrapped. Moreover, a high pouring temperature leads to large undercooling, which is not conducive tothe formation of Type A graphite. If the pouring temperature is too low, it is unfavorable for degassing and will also cause the castings to be too hard and to have cold shuts, unclear contours, and other problems. With an appropriately slightly lower pouring temperature, the liquid shrinkage of the molten iron is smaller, which helps reduce shrinkage cavities and obtain dense castings. Castings with different wall thicknesses and weights have different ideal pouring temperatures. In daily production, the pouring temperature is generally controlled at 1450–1380°C. For thick and large castings, it is necessary to ensure “high-temperature tapping, low-temperature fast pouring”. In order to shorten the waiting time for the molten iron temperature to drop to the pouring temperature and prevent inoculation fading, the molten iron can be rapidly cooled by ladle-to-ladle transfer plus holding, so as to prevent shrinkage porosity and improve production efficiency.

3.3 Control of Sulfur and Nitrogen

Melting cast iron in a medium-frequency induction electric furnace has no sulfur pickup source; the molten iron'sS content is relatively low, which is a great advantage for producing ductile iron. However, for gray iron, low sulfur and relatively high manganese will increase casting stress, greatly increasing the probability of cracks, and an appropriate amount of sulfur in the molten iron can improve the inoculation effect. In the past, when cupolas were used to produce gray iron, because coke would cause sulfur pickup in the molten iron, there was no need to worry about low sulfur. However, when a medium-frequency induction furnace is used to produce gray iron, not only is there no sulfur pickup, but also, because a large amount of steel scrap is used, the S content becomes even lower (about 0.04%). In gray iron, w(S)≤0.06% will lead to poor graphite morphology, difficulty in inoculation, shrinkage porosity, and a high chill tendency. In past production, it was found that castings with cracks and chill defects mostly had graphite morphologies dominated by D and E type graphite. For electric furnace molten iron to obtain normal graphite morphology, it must have an appropriate S content. If sulfur and sulfide contents are low, the number of crystal nuclei will decrease, graphite nucleation ability will decrease, chill will increase, A-type graphite will decrease, D and E type supercooled graphite and ferrite will increase, grains will become coarse, and strength will decrease[4]. Moreover, as the holding time of high-temperature molten iron is prolonged, the degree of supercooling continues to increase. The higher the grade of gray iron, the more significant the influence of holding temperature and time on the degree of supercooling. Some data indicate that molten ironS content is low, the number of eutectic cells is small; as S content increases, the number of eutectic cells increases sharply, and the greater the number of eutectic cells and the finer their size, the better the mechanical properties of cast iron. Therefore, when melting gray iron in a medium-frequency induction furnace, the S content is generally raised to 0.06%–0.10% to give full play to the beneficial role of sulfur, improve the inoculation effect, increase the number of nuclei in the molten iron, make the metallographic structure of the casting mainly A-type graphite, and increase the pearlite content in the matrix structure, thereby improving the strength and machinability of the cast iron. The specific practice is to add FeS to increase sulfur after adjusting the composition in the later stage of melting; coke or anthracite is also used as a carburizer, and while carburizing, the S content is also increased to more than 0.06%. However, the S content must not be too high, because sulfur is an element that hinders graphitization, and too high a content will increase chill. When the S content is appropriately high, as the Mn content increases, the generated MnS fully plays a heterogeneous nucleation role and can create conditions for good inoculation. However, when the Mn content is greater than 1%, excessive MnS is generated and segregates at grain boundaries, weakening the grain boundaries and even producing slag inclusions, reducing the strength of the cast iron. From the perspective of reducing MnS inclusions, the S content should be controlled to less than 0.1%, so that a higher amount of manganese is allowed to exist, which is beneficial for improving the performance of gray iron.

Because a large amount of steel scrap is used in melting gray iron in a medium-frequency induction furnace, and as the proportion of steel scrap increases, the amount of carburizer increases accordingly; in addition, the carburizer contains relatively high nitrogen, so the molten iron in a medium-frequency induction furnace has arelatively high N content. When the N content in molten iron is greater than 100×10-4%, castings are prone to cracking, shrinkage porosity, and fissure-like subsurface blowhole defects[5]. To control the N content in molten iron,the effective method is to hold the molten iron at high temperature, and as the holding time is prolonged, the N content will gradually decrease. However, holding high-temperature molten iron for a long time will increase the degree of supercooling and chill tendency, so in daily production, graphite carburizers with low N content should be selected. When necessary, 10% iron oxide powder can be added to the coating to eliminate the effect of high nitrogen. However, nitrogen in gray iron, like sulfur, is a restricted element; a trace amount of nitrogen in molten iron can refine the grains and eutectic cells of gray iron, increase the amount of pearlite in the matrix, and improve mechanical properties. It can play a positive role in improving the graphite morphology of gray iron and promoting pearlization of the matrix structure. Nitrogen compounds can also act as crystal nuclei, creating growth conditions for graphite nucleation. In actual production, the N content should generally be controlled below 0.008%.

3.4 Enhanced Inoculation Treatment

During inoculation treatment, a large number of artificial crystallization nuclei are added, forcing the cast iron to undergo eutectic solidification under controlled conditions. Its purpose is to promote graphitization, reduce chill tendency and section sensitivity, control graphite morphology, reduce supercooled graphite and associated ferrite, appropriately increase the number of eutectic cells, promote the formation of pearlite, and thereby improve the strength and machinability of the cast iron. Enhanced inoculation treatment in actual production is to select suitable inoculants, inoculation amounts, and inoculation methods, and for carbon equivalentCE of 3.9%–4.1% and a temperature of about 1480°C, perform efficient inoculation on high-temperature molten iron, so as to obtain gray iron castings with good casting performance and high mechanical properties. Different inoculants have different characteristics; it is necessary to reasonably select the inoculant, inoculation amount, and inoculation method according to the characteristics of the inoculant and in combination with the enterprise's own production conditions. After selecting and establishing the treatment method most suitable for the enterprise's characteristics through tests, the process should be strictly controlled to ensure stable casting quality.

In addition to adding inoculant in the stream and controlling the addition amount and stream time, the following aspects should also be noted to prevent inoculation fading and improve the inoculation effect:① Due to the limitations of melting temperature and holding time, the coarse graphite flakes in pig iron cannot be completely dissolved. The incompletely dissolved coarse graphite characteristics will be inherited by the cast iron, greatly offsetting the effect of inoculation. Therefore, in actual production, the amount of pig iron should be minimized to eliminate the heredity of pig iron, improve the inoculation effect, and improve the performance of gray iron; ② Inoculants containing calcium and aluminum and having many refractory heterogeneous nucleation nuclei should be selected, and the inoculant should be controlled to have an appropriate particle size, because the particle size of the inoculant has a very large influence on the inoculation effect. If the particle size is too fine, it is easily oxidized and enters the slag, losing its effect; if the particle size is too large, the inoculant does not melt completely, not only failing to fully exert the inoculation effect, but also causing defects such as segregation, hard spots, and supercooled graphite. The particle size of the inoculant is generally controlled at 3–8 mm (for molten iron amounts below 1 t), and the inoculation amount is generally controlled at about 0.30%–0.55% of the weight of the molten iron. Excessive inoculation amount will increase the shrinkage and slag inclusion tendencies of the cast iron; ③ Multiple inoculation can effectively prevent inoculation fading, improve the uniformity of graphite distribution inside the cast iron, reduce the supercooling tendency of the molten iron, make the proportion of A-type graphite high with moderate length, promote an increase in the number of non-spontaneous nuclei, refine grains, strengthen the matrix, and improve the strength and performance of the cast iron. For example, for secondary inoculation, a Si-Ba long-acting inoculant with a very strong ability to promote graphitization can improve the morphology and distribution of graphite in thin-walled castings, increase eutectic cells, promote the formation of A-type graphite, eliminate supercooled graphite, inhibit the formation of free cementite, and slow down inoculation fading; ④ The influence of molten iron temperature on inoculation is that, within a certain range, increasing the superheating temperature of the molten iron and maintaining it for an appropriate time can completely dissolve the residual undissolved graphite in the molten iron, eliminate the influence of hereditary factors, fully exert the effect of the inoculant, and improve the inoculation receptivity of the molten iron. The superheating temperature is preferably increased to about 1520°C, and the inoculation treatment temperature is preferably controlled at 1460–1420°C.

3.5 Adjustment and Improvement of Process Technology

(1) Process operation sequence for melting gray iron in a medium-frequency induction electric furnace: small pieces of returns and steel scrap + graphite carburizer + steel scrap and new pig iron + returns + ferroalloys + appropriate inoculation. In order to improve the adverse effects caused by high-temperature long-time holding of molten iron, based on the advantages of the medium-frequency induction furnace being easy to raise temperature and capable of rapid melting, a “fast melting and fast tapping” process operation method is formulated, so as to shorten the melting time as much as possible, accelerate the melting speed, make the molten iron be tapped as soon as possible after chemical composition adjustment and temperature rise in the furnace, and accelerate the pouring speed, striving to complete pouring in about 5 min, and minimizing the holding time of molten iron in the furnace and ladle.

(2) Slag inclusions have a great impact on casting quality. In light cases, fine slag inclusions split the matrix and reduce tensile strength; in severe cases, slag inclusion defects can directly cause castings to be scrapped. After the charge containing more slag inclusions is melted, the slag inclusions attached to the furnace wall and existing in the molten iron float up one after another under the action of electromagnetic stirring of the electric furnace and the buoyancy of the molten iron. In the later stage of melting, slag must be skimmed frequently and efficiently. Especially when impurities float up during high-temperature standing, slag should be skimmed in time until the surface of the molten iron is clean and no new floating slag appears. This is very important for removing slag inclusions, eliminating slag hole defects, and reducing the destructive effect of slag inclusions on the matrix.

(3) Because the medium-frequency induction furnace melting of gray cast iron uses a large amount of steel scrap and returned iron, on the one hand it will promote the formation of dendritic graphite in cast iron and increase the chill tendency, raise hardness, and worsen machinability. Therefore, more attention should be paid to inoculation than with cupola molten iron, so as to promote graphitization, refine eutectic cells, change graphite morphology, reduce the chill tendency, transform white or mottled structure into fine pearlite structure, transform type D and E graphite into uniformly distributed type A graphite, improve the uniformity of structure at different wall thicknesses of castings, and achieve the purpose of improving cast iron performance. On the other hand, the increase in steel scrap amount lowers the S content of the molten iron; when w(S)≤0.06%, it easily leads to inoculation difficulties[6], generally usingFeSi75 inoculation treatment has no obvious effect, and sulfur-increasing measures should be taken.

(4) Thin-wall castings have severe chill defects, are difficult to machine, and have a high reject rate. To solve this prominent problem, first of all, the use of alloy steel scrap must be prohibited, and CE should be appropriately increased[7], and control, before treatment, the molten iron'sSi content at 1.6% or more, S content greater than 0.06%, increase the inoculation amount to 0.55%, so that the number of nuclei in the molten iron increases, the graphite nucleation ability improves, the formation of type A graphite is promoted, the generation of type D and E graphite is inhibited, the amount of pearlite in the matrix structure increases, the undercooling and chill tendency of the cast iron decrease, and the strength and machinability are improved. Reasonably controlling the microstructure of gray cast iron is the key to improving the machinability of gray cast iron. When necessary, 2% clean, rust-free small pieces of pig iron can be added to the ladle before tapping, effectively increasing graphite particles and eliminating chill. 4 Some views on improving the quality and performance of gray cast iron castings. People in the industry all know that domestic castings and imported castings with basically the same chemical composition and basically consistent metallographic analysis differ greatly in service performance and surface finish; imported castings with the same carbon equivalent are 1–2 grades higher than domestic castings; imported castings with higher hardness than domestic castings are instead superior to domestic castings in machinability. The reasons for these phenomena are that imported castings have higher material purity and carbon equivalent, fewer inclusions and free carbides, and better structural uniformity. The internal quality, appearance quality, and whether casting defects will form in cast iron castings are closely related to various factors of the molten iron. High-quality molten iron is the most basic and most important prerequisite for obtaining high-quality cast iron castings. Molten iron quality is in turn determined by factors such as molten iron temperature, chemical composition, and purity. In medium-frequency induction furnace melting of gray cast iron, it is very easy to obtain molten iron with a high temperature above 1500°C and precise chemical composition. Each element in the molten iron has a certain influence and effect on the solidification and crystallization, structure, and properties of cast iron; the level of molten iron superheating temperature can directly affect the composition and purity of the molten iron. Increasing it within a certain range can refine graphite, make the matrix structure dense, increase tensile strength, improve casting performance, and also make impurities in the molten iron easier to float up and be removed by slagging. Only the purity of molten iron still remains at the levels of high-temperature melting, slag coagulants, and filter screens. In fact, experts in the industry all understand that through these measures it is difficult to obtain highly clean molten iron; they can only improve the situation. However, there is little research and few countermeasures for deep purification of molten iron, analysis of the occurrence mechanism of casting defects, and prevention. Various harmful gases and non-metallic inclusions present in the molten iron remain in the castings after the molten iron solidifies, causing various casting defects and affecting the service performance of the castings; hard particles formed by non-metallic inclusions make castings difficult to machine; and impurity harmful elements contained in the molten iron directly affect the structure and properties of the castings. It is precisely these factors that have caused the comprehensive quality of domestic cast iron castings to remain lower than that of imported castings for a long time. Therefore, we should vigorously improve the metallurgical quality of molten iron, strive to obtain highly clean molten iron with low harmful element and gas content and few inclusions, and on the basis of the current gray cast iron medium-frequency induction electric furnace melting process, further perfect modern molten iron purification technology and process flow, ensuring that the molten iron used for pouring must be highly pure molten iron, thereby ensuring the high quality and high performance of castings.

 

5 Conclusion

(1)In medium-frequency induction electric furnace melting of gray cast iron, steel scrap must have a certain proportion, generally accounting for more than half of the charge. Low-nitrogen graphite carburizer should be selected, and a high carburization rate ensured, so as to obtain high-quality molten iron with good graphitization degree and low chill and shrinkage porosity tendencies. At the same time, use a large amount of steel scrap and returned iron, and use little or no new pig iron, to eliminate the hereditary influence of coarse graphite. Also, by utilizing the price difference between pig iron and steel scrap and melting during the nighttime low electricity price period, production costs can be greatly reduced.

(2)In medium-frequency induction furnace molten iron,S content is generally relatively low, so sulfur-increasing measures should be taken to raise the S content of the molten iron to 0.06%–0.10%, increase nucleation ability, increase the number of crystal nuclei and pearlite content, improve graphite morphology, and refine graphite, promote the formation of type A graphite, improve inoculation effect and machinability, and increase strength.

(3)By adopting the steel scrap carburization process+ appropriately increasing CE and the Si/C ratio + the operating method of fast melting and fast tapping + strengthening inoculation treatment and other production technologies, controlling the molten iron superheating temperature at 1510–1530°C and the tapping temperature at 1480–1500°C, to achieve the purpose of reducing casting defects, enhancing gray cast iron performance, improving molten iron quality and casting quality, and reducing the reject rate.

(4)Molten iron quality is an important factor affecting the quality of cast iron castings. Without high-quality molten iron, there can be no high-quality castings. On the basis of the current medium-frequency induction furnace gray cast iron melting process, efforts should be made to improve the purity of the molten iron and further perfect modern molten iron purification technology and process flow, so as to ensure the high quality and high performance of gray iron castings.

 

References:

[1] Lu Wenhua, Li Longsheng, Huang Liangyu. Casting Alloys and Their Melting [M]. Beijing: China Machine Press, 2008.

[2] Tong Jun, Zhang Zhou, Lian Wei. Cast Iron Induction Electric Furnace Melting and Application Examples [M]. Beijing: Chemical Industry Press, 2008.

[3] Zou Rongjian, Xie Zhaichuan. Application of All-Steel-Scrap Technology in Cast Iron Production [J]. Foundry Technology, 2008(12): 1747-1748.

[4] Yue Hai, Zhao Chaoyun. Control of Graphite in High-Strength Gray Cast Iron Melted in a Medium-Frequency Furnace [J]. Foundry Equipment and Technology, 2013(4): 42-44.

[5] Yin Zuohu. Effect of Sulfur on the Structure and Properties of Gray Cast Iron [J]. Foundry, 2004, 53(10): 805-809.

[6] Shen Zhongren, Shi Yongde, Liu Dangku. Casting Defects Easily Produced in Molten Iron Melted in a Medium-Frequency Furnace and Preventive Countermeasures [J]. Foundry Technology, 2012(6): 744-746.

[7] Lin Yanru, Li Yanqin. Effect of Carbon Equivalent on Machinability of Cast Iron and Its Control [J]. Metal Working-Hot Working, 2014(13): 46-48.